Dissolution, Hydrolysis and Crystallization Behavior of Polyamide 6 in Superheated Water
PAPER|Updated:2021-06-21
|
Dissolution, Hydrolysis and Crystallization Behavior of Polyamide 6 in Superheated Water
Dissolution, Hydrolysis and Crystallization Behavior of Polyamide 6 in Superheated Water
Chinese Journal of Polymer Science2015年33卷第9期 页码:1334-1343
Affiliations:
a.State Key Laboratory for Modification of Chemical Fibers and Polymer Materials, College of Material Science and Engineering, Donghua University, Shanghai 201620, China
b.R & D Center, Guangdong Xinhui Meida Nylon Co., LTD., Jiangmen 529100, China
c.Department of Mathematics and Physics, Chongqing University of Posts and Telecommunications, Chongqing 400065, China
Author bio:
**Shu-guang Yang (杨曙光), E-mail: shgyang@dhu.edu.cn
Funds:
the National Natural Science Foundation of China(51373032);Innovation Program of Shanghai Municipal Education Commission, Fundamental Research Funds for the Central University and DHU Distinguished Young Professor Program. Z.W. thanks the support from Chinese Universities Scientific Fund(CUSFDH-D-2014025)
Zhi-liang Wang, Jia-li Xu, Lian-jia Wu, 等. Dissolution, Hydrolysis and Crystallization Behavior of Polyamide 6 in Superheated Water[J]. Chinese Journal of Polymer Science, 2015,33(9):1334-1343.
Zhi-liang Wang, Jia-li Xu, Lian-jia Wu, et al. Dissolution, Hydrolysis and Crystallization Behavior of Polyamide 6 in Superheated Water[J]. Chinese Journal of Polymer Science, 2015, 33(9): 1334-1343.
Zhi-liang Wang, Jia-li Xu, Lian-jia Wu, 等. Dissolution, Hydrolysis and Crystallization Behavior of Polyamide 6 in Superheated Water[J]. Chinese Journal of Polymer Science, 2015,33(9):1334-1343.DOI: 10.1007/s10118-015-1682-3.
Zhi-liang Wang, Jia-li Xu, Lian-jia Wu, et al. Dissolution, Hydrolysis and Crystallization Behavior of Polyamide 6 in Superheated Water[J]. Chinese Journal of Polymer Science, 2015, 33(9): 1334-1343.DOI: 10.1007/s10118-015-1682-3.
Dissolution, Hydrolysis and Crystallization Behavior of Polyamide 6 in Superheated Water
crystallization and hydrolysis behaviors of polyamide 6 (PA 6) in superheated water (140 ℃≤
T
H
≤ 200 °C) are investigated. The hydrothermal processing of PA 6 can be divided into four regions: (I)
T
H
<
140 °C
(II) 140 ℃≤
T
H
≤ 155 °C
(III) 155 ℃
<
T
H
<
160 ℃and (IV)
T
H
≥ 160 °C. Below 140 °C
the hydrothermal processing does not have obvious impact on PA 6. Between 140 ℃and 155 °C
an annealing effect is observed that the hydrothermally treated resin shows increased melting temperature and lamellar thickness compared with the original PA 6. Between 155 ℃and 160 °C
the hydrothermal processing induces both annealing and surface swelling. Above 160 °C
PA 6 dissolves fully in the superheated water. As PA 6 dissolves in the superheated water
hydrolysis takes place and becomes more prominent at higher temperatures and longer processing time. The hydrolysis induced molecular weight decrease fits an exponential decay.